The Mechanical Properties of Beta-Quenched Uranium at Elevated Temperatures (open access)

The Mechanical Properties of Beta-Quenched Uranium at Elevated Temperatures

The creep strength and tensile properties-were determined in vacuum for beta-quenched, derby uranium. The stresses to produce a secondary creep rate of- 0.0001 per cent per hr at 100, 250, 400, and 500 deg C were 48,000, sile strengths were 114,500, 35,100, 11,100, and 8,500 psi at temperatares of 28, 300, 500, and 700 deg C, respectively. The creep and tensile strengths decrease quite rapidly with increasing temperature in the temperatare range 250 to 400 deg C.
Date: September 6, 1955
Creator: Shober, Frederic R.; Marsh, Lyle L. & Manning, G. K.